National Electroless Nickel - ISO American Global Standards

Specifications & Properties

Low Phosphorus Electroless Nickel


Low Phosphorus Electroless Nickel Our Low Phosphorus Electroless Nickel process meets the requirements of ASTM B733 class V, AMS 2404, mil C26074 (all revisions), and ISO 4527. The coating conforms to the requirements of ELV Directive 2000/53/EC, WEEE 2002/96/EC, RoHS 2002/95/EC and NSF/ANSI 51-2005. IMDS number 32692646



LOW PHOSPHORUS PHYSICAL PROPERTIES Typical Result
Phosphorus Content, wt, % 2 to 4
Melting Point (eutectic) 1706 to 2057 °F
930 to 1125 °C
Coefficient of Thermal Expansion, °m/(mK) 13 to 15
Thermal Conductivity, W/(mK) 44 to 57
Electrical Resistivity μΩ/ cm
(Heat Treated @ 350 °C/1hr.)
30 to 50
10 to 20
Magnetic Properties Magnetic
Hardness, Vickers hardness HV0.1, 100 g load, 40 μm deposit, steel
As plated 670 to 700
Heat Treated @
16 hr., 535 °F (280 °C) 970 to 1030
4 hr., 660 °F (350 °C) <985 to 1045
1 hr., 750 °F (400 °C) 985 to 1045
Wear Properties, Taber Abraser Wear Test, Index Value weight loss mg/1000 cycles CS 10
As Plated 4 to 6
Heat Treated @ 1 hr., 750 °F (400 °C) 2 to 4
Corrosion Related Properties (25 μm thickness; Rz 1.5 μm; base material St 52.3)
DIN ISO EN 50021 SS (hr.) 48 to 96










Your satisfaction is our business!